Steel Grade

1.4310 - 301 HT5

STANDARDS

CHEMICAL COMPOSITION %

C

Mn

Si

P

S

Cr

Ni

Mo

N

Ti

Cu

Co

OTHER

EN 10088-2

0.05-0.15

max
2.0

max
2.0

max
0.045

max
0.015

16.00-19.00

6.0-9.5

max
0.80

max
0.11

 

ASTM A 240

max
0.15

max
2.0

max
1.0

max
0.045

max
0.03

16.0-18.0

6.0-8.0

max
0.10

 

OTELINOX

0.095

1.05

1.1

0.025

0.002

16.8

6.5

0.2

0.01

 

 

EUROPE TYPE

USA TYPE

OTELINOX TYPE

PRACTICABILITY

Corrosion resistance

Cold forming

Weldability

Mechanical strength level

Resistance of hot oxidation

Utilizations

1.4310

301

301HT5

***

***

***

*****

*

Automotive industry, chemical industry, building tools, decorative purposes, tubes, soles for safety shoes, gaskets, springs, pot lid, connectors, watch parts

* Low; **Medium; *** Good; **** Very good; ***** Excellent.

STANDARDS

MECHANICAL PROPERTIES AT AMBIENT TEMPERATURE IN ANNEALED CONDITION

SURFACE FINISH

0.2% Proof strength

1% Proof strength

Tensile strength

Elongation %

Hardness

N/mm2

HB

HRB

EN 10088-2

2B & 2R

≥250

≥280

600-950

≥40

  

ASTM A 240

2B & BA

≥205

≥515

≥40

≤217

≤95

OTELINOX

2B

300-410

760-920

40

79-93

2R & BA

325-410

760-920

40

79-93

 

MECHANICAL PROPERTIES IN COLD-WORKED CONDITION
(According to EN 10088 and EN 10151 standards)

MECHANICAL PROPERTIES

C700

[700-850)

C850

[850-1000)

C1000

[1000-1150)

C1150

[1150-1300)

C1300

[1300-1500)

C1500

[1500-1700)

C1700

[1700-1900)

C1900

[1900-2200]

0.2% Proof strength

≥650

≥800

≥1200

≥1500

Elongation %

≥15.0

≥10.0

≥3.0

≥1.0

Hardness

 

MECHANICAL PROPERTIES IN COLD-WORKED CONDITION (According to ASTM A 666)

ASTM

OTELINOX

SURFACE FINISH

TENSILE STRENGTH (N/mm2)

0.2% Proof str. [N/mm2]

Elongation [%]

Hardness [HV]

1/4H

860-1034

1/2H

1035-1204

≥540

23.0-40.0

3/4H

1205-1274

≥650

19.5-31.5

Full Hard

≥1275

≥750

1.0-23.0